国产精品福利电影-国产精品福利电影一-国产精品福利短视在线播放-国产精品福利短视在线播放频-国产精品福利久久-国产精品福利久久2025

ChineseEnglish Hotline:0571-86062609
Industry information current location:Home  > News > Industry information
Aluminum Foil Click rate: Release time:2022-01-25 Information sources:Hangzhou Qiyao New Material Co.,Ltd.

Although there are many kinds of aluminum foil rolling defects, they are mainly manifested as: pinhole, roll hole, seam opening and air passage characterized by holes; Oil stains, uneven luster, vibration marks, tension lines, water spots and bright spots characterized by surface conditions; In order to affect the shape of the plate, wrinkle, discount, bad coiling process; A thickness difference characterized by size. In essence, aluminum foil unique defects only a kind of pinhole, several other defects of the plate also have the same, but the performance of the severity of different or different requirements.

1.pinhole. Pinhole is the main defect of aluminum foil. Raw materials, rolls, rolling oil, and even dust in the air size of about 6μm into the roll gap will cause pinholes, so 6μm aluminum foil without pinholes is impossible, can only be evaluated by how much and size. Due to the improvement of aluminum foil rolling conditions, especially the effective filtration of dust and rolling oil and the setting of convenient roll change system, the number of aluminum foil pinholes increasingly depends on the metallurgical quality of raw materials and processing defects, because pinholes are often raw material defects fall off, it is difficult to find the corresponding relationship with the original defects. It is generally believed that pinholes are mainly related to gas content, inclusions, compounds and component segregation. Effective purification, filtration and grain refinement of liquid aluminum are helpful to reduce pinhole. Of course, alloying and other means to improve the hardening properties of materials can also help reduce pinhole. High quality hot rolled material rolling 6μm aluminum foil pinholes can be less than 100 /㎡. When the purification is good, 6μm aluminum foil pinholes in 200 / square meters or less. Other causes of pinholes in the aluminum foil rolling process are numerous, even catastrophic, and thousands of pinholes per square meter are not uncommon. Effective filtering of rolling oil, short-term change of roll and dustproof measures are necessary conditions to reduce pinholes in aluminum foil, and large rolling force and small tension rolling will also help to reduce pinholes.

2.roll printing, roll eye, uneven luster. It is mainly caused by roller aluminum foil defects, divided into point, line, surface three. The main reasons for this defect are: incorrect grinding of roll; Foreign material damage roll: incoming material defect imprint injury roll; Roll fatigue; Roller impact, skid, etc. All the factors that can cause roller surface damage can be harmful to aluminum foil rolling. Because aluminum foil rolling roll surface finish is very high, slight gloss uneven will also affect its surface state. Regular cleaning of the rolling mill, keeping the rolling mill clean, ensuring the normal work of the roller cleaner, regular roll change, reasonable grinding, are the basic conditions to ensure the uniform surface of aluminum foil rolling.

3. wrinkle. Because of the serious bad shape, when the aluminum foil is rolled or expanded, wrinkle will be formed. Its essence is that the tension is not enough to flatten the foil surface. For the device with a tensile dimension of 20MPa, the shape of the foil surface shall not be greater than 30I, when greater than 30I, it is bound to wrinkle. Because the aluminum foil is often subjected to more tension than the subsequent processing, some in the rolling performance is only bad shape, including roller grinding is not correct, roll type is not correct, the incoming plate shape and adjust the plate shape is not correct.

4. The thickness difference. The thickness difference is difficult to control is a characteristic of aluminum foil rolling. 3% thickness difference may not be difficult in plate production, but it is very difficult in aluminum foil production. The reason is that the thickness is thin, and other microconditions can affect, such as temperature, oil film, oil and gas concentration, etc. Aluminum foil rolling a roll can reach hundreds of thousands of meters, rolling time up to 10h or so, with time extension, the thickness difference is easy to form, and the means of thickness adjustment only tension speed. All these factors have caused the difficulty of thickness control of aluminum foil rolling, so it needs many conditions to ensure that the thickness difference is really controlled within 3%, which is quite difficult.



Copyright ? 2017 qiyaomaterial.com All Rights Reserved Copyright·Hangzhou Qiyao New Material Co.,Ltd. Zhejiang ICP No. 17034714-1
主站蜘蛛池模板: 日韩国产精品一区二区 | 成人免费一区二区三区视频软件 | 亚洲都市校园激情另类 | 欧美日韩高清不卡一区二区三区 | 亚洲av午夜福利精品一区二区 | 无码国产精品一区二区色情男同 | 亚洲中文字幕无码 | 欧美一级做a爰片免费 | 国产乱色国产精品播放视频 | 免费国产美女爽到喷出水来视频 | 免费的又色又爽又黄的视频软件 | 国产一区二区三区不卡av | 国产色99在线新视频 | 亚洲线精品久久一区二区三区 | 国产欧美亚洲日韩图片 | 91欧美激情一区二区三区成人 | 日本欧美久久久久免费播放网 | 中文字幕无码不卡一区二区 | 久久国内精品自在自线图片 | 欧美精品一区二区在线观看 | 亚洲国产精品无码久久久秋霞2 | 新国产精品视频福利免费 | 国产无码高清在线观看 | 国产成人精品亚洲一区 | 欧美午夜色情高清苦月亮 | 国产亚洲欧美精品久久久 | 国产高跟黑色丝袜在线 | 日韩成人无码影院 | 亚洲精品国产品国语原创 | 亚洲伊人久久成综合人影院 | 欧美成人禁片在线观看 | 国产无码黄色网站在线观看 | 久久久久久国产精品免费网站 | 精品视频免费播放 | 亚洲欧美日韩二页 | 久久国产伦子伦精品 | 亚洲av日韩精品久久久久久 | 国产国产精品人在线观看 | 在线观看国产一区二区三区不卡 | 人妻洗澡被强公日日澡电影 | 日韩欧美精品亚洲一级在线 |